ASTM A179 / ASME SA179 Heat Exchanger Tubes

Nov 28, 2025 Leave a message

ASTM A179 and its ASME counterpart SA179 specify minimum-wall seamless cold-drawn low-carbon steel tubes for tubular heat exchangers, condensers and similar heat-transfer apparatus. ASME SA179 is the same specification adopted for ASME boiler and pressure vessel code construction, so the technical content a purchaser buys is identical; what changes is the certification context. The grade is defined by a low carbon range, a low hardness ceiling and cold-drawn tolerances, all of which serve one purpose: a tube that can be rolled or expanded into a tubesheet and kept clean in heat-transfer service. This page brings the specification together in one place, from the ASME adoption through the size range, chemistry, tolerances and hydrostatic test bands that appear on every order.

How ASTM A179 and ASME SA179 relate

Every ASME specification that begins with SA is an ASTM specification adopted into Section II of the ASME Boiler and Pressure Vessel Code, and SA179 is the adopted version of ASTM A179. The requirements for chemistry, mechanical properties, tolerances and testing are the same; the SA designation simply signals that the material is acceptable for code construction and will be certified within the code's traceability rules. In practice a purchaser working to a plant code built on ASME references orders SA179 and receives mill paperwork carrying that designation, while a purchaser working to ASTM standards orders A179. Suppliers who produce the tube normally certify to either designation from the same production route: piercing, cold drawing and a stress-relief heat treatment at 1200 degrees F (650 degrees C) or higher after the final draw. The essentials of the tube and its product page are summarized on the A179/SA179 heat exchanger tubes page.

Point ASTM A179 ASME SA179
Origin ASTM standard specification ASTM A179 adopted by ASME Section II
Technical content Full specification requirements Identical requirements to A179
Certification context General ASTM purchase ASME boiler and pressure vessel code construction
Mill paperwork Certificate cites A179 Certificate cites SA179
Production route Piercing, cold drawing, stress relief Same route, same values

Scope and size range

The specification covers tubes from 1/8 in to 3 in outside diameter, which is 3.2 mm to 76.2 mm, delivered on a minimum-wall basis. Two boundary rules matter when reading drawings. First, tubes with wall thickness below 0.015 in (0.4 mm), or with outside diameter below 1/8 in, are not subject to the mechanical-property requirements of the specification, so a certificate for such tubes will not carry tensile or hardness values. Second, the specification calls for minimum wall, not nominal wall: the ordered wall is the floor, and the published tolerance allows the wall to run heavier from there. This is the opposite of schedule-based pressure pipe and is one of the quickest ways to tell an A179 enquiry from an A106 enquiry.

Dimension rule Requirement
Outside diameter range 1/8 in to 3 in (3.2 to 76.2 mm)
Wall basis Minimum wall delivery
Very light walls Below 0.015 in (0.4 mm) wall, mechanical requirements do not apply
Very small tubes Below 1/8 in OD, mechanical requirements do not apply
General requirements ASTM A450/A450M

Chemistry and mechanical properties

The chemistry is a plain low-carbon composition: carbon between 0.06 and 0.18 percent, manganese between 0.27 and 0.63 percent, and phosphorus and sulfur each at 0.035 percent maximum. No deliberate alloy additions are made. The mechanical requirements are a minimum tensile strength of 325 MPa (47 ksi), a minimum yield of 180 MPa (26 ksi), minimum elongation of 35 percent and a hardness ceiling of 72 HRB. Heat treatment is fixed at 1200 degrees F (650 degrees C) or higher after the final cold draw, as a stress relief rather than a normalizing treatment. The hardness ceiling deserves attention in any specification review, because it is the property that lets the tube be rolled into a tubesheet without cracking and gives the joint its leak-tight behavior.

Requirement Value Purpose
Carbon 0.06 to 0.18% Ductility for drawing and tube rolling
Manganese 0.27 to 0.63% Modest strength without hardening
Phosphorus and sulfur 0.035% max each Clean steel for surface and joint quality
Tensile strength 325 MPa (47 ksi) min Baseline for heat-transfer service
Yield strength 180 MPa (26 ksi) min Consistent with low-carbon design
Elongation 35% min Forming and expanding capability
Hardness 72 HRB max Tube rolling into tubesheets without cracking

Tolerances: the numbers that decide fit-up

For cold-drawn bright tube, the wall tolerance is plus 20 percent with zero undersize for outside diameter up to and including 1.5 in (38.1 mm), and plus 22 percent with zero undersize above that size. Outside diameter tolerance is banded in five steps across the size range, from plus or minus 0.004 in (0.1 mm) on tubes below 1 in to plus or minus 0.012 in (0.3 mm) in the 2.5 to 3 in band. These figures are what a tubesheet hole design works against, so they appear on nearly every exchanger drawing. The one-directional wall tolerance is deliberate: minimum wall can run heavy but never light, which protects the pressure calculation while allowing the rolling tolerance to do its work.

Outside diameter band OD tolerance Wall tolerance
Below 1 in (25.4 mm) Plus or minus 0.004 in (0.1 mm) Plus 20%/0 up to 1.5 in OD
1 to 1.5 in Plus or minus 0.006 in (0.15 mm) Plus 20%/0 up to 1.5 in OD
1.5 to 2 in Plus or minus 0.008 in (0.2 mm) Plus 22%/0 above 1.5 in OD
2 to 2.5 in Plus or minus 0.010 in (0.25 mm) Plus 22%/0 above 1.5 in OD
2.5 to 3 in Plus or minus 0.012 in (0.3 mm) Plus 22%/0 above 1.5 in OD

Testing, including the hydrostatic pressure bands

Each batch is tested for tension, flattening, flaring and hardness, and every tube is proved either by hydrostatic test or, when the order agrees, by a nondestructive electrical method such as eddy current. The hydrostatic test pressure is banded by outside diameter: 1000 psi for tubes below 1 in, 1500 psi from 1 to 1.5 in, 2000 psi from 1.5 to 2 in, and 2500 psi from 2 to 3 in. The flattening and flaring tests exist because the tube will be deformed in service assembly, and the hardness test confirms that the stress relief restored ductility after the final draw. Surface condition is part of acceptance too: tubes are supplied free of scale, and a slight oxidation film after heat treatment does not count as scale, while ends are cut flat and deburred for tubesheet work. These requirements and the size bands are shown in product form on the A179/SA179 heat exchanger tube page.

Tube OD band Hydrostatic test pressure
Below 1 in 1000 psi
1 to 1.5 in 1500 psi
1.5 to 2 in 2000 psi
2 to 3 in 2500 psi

Need SA179 or A179 tube with full traceability?

State the designation your code requires, together with size, wall and test expectations, and the certificate will match the order from the first shipment. Request a quotation.

Frequently Asked Questions

Are ASTM A179 and ASME SA179 the same material?

Yes. SA179 is ASTM A179 adopted into the ASME Boiler and Pressure Vessel Code. The chemistry, mechanical properties, tolerances and tests are identical; only the certification context and the designation on the certificate differ.

Which designation should I order?

Order SA179 when your construction code is built on ASME Section II and the paperwork must cite the SA designation. Order A179 for general ASTM purchases. Both come from the same production route and the same values.

What sizes does the specification cover?

Outside diameters from 1/8 in to 3 in, which is 3.2 mm to 76.2 mm, on minimum-wall delivery. Tubes with wall below 0.015 in or outside diameter below 1/8 in are outside the mechanical-property requirements.

Why is the wall tolerance one-directional?

The specification calls for minimum wall, so the wall may run heavier by 20 or 22 percent but never below the ordered value. That protects the pressure calculation while allowing cold-drawing practice its working band.

What hydrostatic test pressure applies to my tube size?

The pressure is banded by outside diameter: 1000 psi below 1 in, 1500 psi from 1 to 1.5 in, 2000 psi from 1.5 to 2 in, and 2500 psi from 2 to 3 in, with an agreed nondestructive electrical test allowed as an alternative.

Does the specification require normalizing?

No. Tubes are heat treated at 1200 degrees F, which is 650 degrees C, or higher after the final cold draw as a stress relief. The specification does not claim grain refinement, and the treatment should not be described as normalizing.

test