What is ASTM A179 specification? In one sentence: A179/A179M is the ASTM product specification for minimum-wall tubes, seamless and cold drawn, in low-carbon steel destined for tubular heat exchangers, condensers and comparable heat-transfer duty, covering outside diameters from 3.2 mm to 76.2 mm and requiring heat treatment at 650 degrees C or higher after the final cold-draw pass. This overview answers the questions a purchaser meets first: what the scope includes, which chemistry and properties are mandatory, what the heat treatment clause really means, which tolerances and tests apply, and how the grade differs from A106 Grade B pressure pipe.
What does the scope of ASTM A179 cover?
The scope names the product form precisely. A179 covers seamless tubes, so there is no weld seam; the tubes are cold drawn to final size; the wall is supplied on a minimum-wall basis; and the named application is heat-transfer apparatus such as tubular heat exchangers and condensers. General requirements for delivery, testing and marking come from ASTM A450/A450M, the companion standard for carbon and low-alloy steel tubes, so an order always references the product specification together with the general requirements standard. Tubes are supplied in straight lengths or as U-bent tubes for exchanger bundles. If you need the supply details behind this scope, the ASTM A179 pipe product page lists the manufactured range.
| Scope item | What the specification states |
|---|---|
| Product | Minimum-wall seamless cold-drawn low-carbon steel tube |
| Application | Tubular heat exchangers, condensers and similar heat-transfer apparatus |
| Size range | 1/8 in to 3 in outside diameter (3.2 to 76.2 mm) |
| Wall basis | Minimum wall, with a plus-only thickness tolerance |
| General requirements | ASTM A450/A450M governs delivery, testing and marking |
Which chemistry and mechanical properties are mandatory?
The chemistry is deliberately narrow. Carbon sits between 0.06 and 0.18 percent: the lower bound guards against steel too soft to hold a finished surface, and the upper bound keeps the tube readily cold drawable and weldable without excessive hardness. Manganese between 0.27 and 0.63 percent provides strength without impairing ductility, while phosphorus and sulfur are held to 0.035 percent max each. On the mechanical side the specification asks for at least 325 MPa (47 ksi) of tensile strength and 180 MPa (26 ksi) of yield strength, elongation of 35 percent or more, and a hardness ceiling of 72 HRB. The low numbers are the point: A179 is chosen for formability, not for strength.
| Requirement | Mandatory value |
|---|---|
| Carbon | 0.06 to 0.18 percent |
| Manganese | 0.27 to 0.63 percent |
| Phosphorus, max | 0.035 percent |
| Sulfur, max | 0.035 percent |
| Tensile strength, min | 325 MPa (47 ksi) |
| Yield strength, min | 180 MPa (26 ksi) |
| Elongation, min | 35 percent |
| Hardness, max | 72 HRB |
What does the heat treatment clause actually mean?
Two clarifications prevent most misunderstandings here. First, the requirement: after the last cold-drawing pass every tube receives heat treatment at 1200 degrees F (650 degrees C) or above. Second, what the treatment is and is not. It is a stress relief, applied to remove the cold work introduced by drawing, restore elongation and bring hardness within the 72 HRB limit. It is not a normalizing treatment for grain refinement, and the specification does not offer a menu of annealed, normalized or tempered conditions. Tubes that are bent after delivery, such as U-bends, are formed cold, and any additional stress relief where the application requires it is a matter for the order. The hardness test on the finished tube is the acceptance check that the relief was effective.
| Question | Answer under the specification |
|---|---|
| When is heat treatment applied? | After the final cold-drawing pass |
| At what temperature? | 1200 degrees F (650 degrees C) or higher |
| What is its purpose? | Relieve cold work, restore elongation, meet 72 HRB max |
| Is it normalizing? | No. It is stress relief, not grain refinement |
| How is it verified? | Hardness test on the finished tube |
Which tolerances and tests apply?
Outside diameter tolerance on cold-drawn bright tube follows five size bands, tightening as the tube gets smaller. Wall thickness carries a plus-only allowance above the ordered minimum, 20 percent on tubes up to 1.5 in outside diameter and 22 percent above that, with the wall never below the ordered minimum. Testing combines lot and individual checks: each lot is tested for tension, flattening, flaring and hardness, and every tube is hydrostatically tested or examined by a nondestructive electric method such as eddy current inspection, as the order states. The surface of the finished tube is required to be free of scale, and ends are cut square and deburred.
| Outside diameter range | OD deviation | Requirement basis |
|---|---|---|
| Under 1 in (25.4 mm) | ±0.004 in (0.10 mm) | Cold-drawn bright tube |
| 1 in to 1.5 in, excl | ±0.006 in (0.15 mm) | Cold-drawn bright tube |
| 1.5 in to 2 in, excl | ±0.008 in (0.20 mm) | Cold-drawn bright tube |
| 2 in to 2.5 in, excl | ±0.010 in (0.25 mm) | Cold-drawn bright tube |
| 2.5 in to 3 in, incl | ±0.012 in (0.30 mm) | Cold-drawn bright tube |
How does A179 differ from A106 Grade B?
A106 Grade B is the comparison buyers raise most often, because both products are seamless carbon steel. The difference starts with scope: A106 is pressure pipe for high-temperature service, transporting steam, water and gas, while A179 is heat-transfer tube for exchangers and condensers. The numbers follow the duty. A106 Grade B allows up to 0.30 percent carbon and 0.29 to 1.06 percent manganese, with a minimum tensile of 415 MPa (60 ksi) and a minimum yield of 240 MPa (35 ksi); A179 caps carbon at 0.18 percent and its strength floor is 325 MPa tensile and 180 MPa yield. A106 is produced hot finished or cold drawn for pressure containment, whereas A179 is always cold drawn and stress relieved for formability. The two are not interchangeable, and where pressure piping is the duty, the A106 Grade B pipe specification page explains that product in full.
| Point of comparison | ASTM A179 | ASTM A106 Grade B |
|---|---|---|
| Named duty | Heat exchanger and condenser tube | High-temperature pressure pipe |
| Carbon limit | 0.06 to 0.18 percent | 0.30 percent max |
| Tensile strength, min | 325 MPa (47 ksi) | 415 MPa (60 ksi) |
| Yield strength, min | 180 MPa (26 ksi) | 240 MPa (35 ksi) |
| Typical process | Cold drawn, stress relieved at 650 degrees C or higher | Hot finished or cold drawn |
Looking for tubes that fully meet ASTM A179?
Send the size, wall, length and test requirements for your exchanger or condenser project and we will confirm compliance and delivery. Request a quotation.
Frequently Asked Questions
What is ASTM A179 specification?
A179/A179M is the ASTM product standard that governs minimum-wall cold-drawn seamless tube in low-carbon steel for heat exchangers, condensers and comparable heat-transfer duty across a 3.2 mm to 76.2 mm outside diameter range, with general requirements taken from ASTM A450/A450M.
What heat treatment does A179 require?
Tube must be heat treated at 650 degrees C or higher after the final cold-drawing pass. The treatment relieves cold work and restores elongation; it is a stress relief, not a normalizing treatment for grain refinement.
How hard can A179 tube be when delivered?
72 HRB is the ceiling. Reading hardness after heat treatment is the acceptance check: a result inside the limit proves the cold work has been relieved, so the tube can be rolled, bent and expanded into tubesheets without cracking.
Why is A179 weaker than A106 Grade B?
Because it serves a different duty. A179 is a heat-transfer tube selected for formability, with minimums of 325 MPa tensile and 180 MPa yield, while A106 Grade B is pressure pipe with minimums of 415 MPa and 240 MPa for containment at high temperature.
Is a hydrostatic test mandatory for every tube?
Every tube must be pressure tested, either hydrostatically or, when the purchaser specifies it in the order, by a nondestructive electric test such as eddy current inspection.
How is A179 tube ordered?
By outside diameter and minimum wall, together with length, test method preference and any marking or packing requirements, referencing the A450/A450M general requirements standard that the specification points to.