Anti-Corrosion Measures for OCTG Casing in Water Injection Wells

Mar 11, 2024 Leave a message

Why OCTG Casing Corrodes in Water Injection Service

Water injection wells place casing and tubing under a combination of oxygen-bearing injection water, dissolved salts, sulphate-reducing bacteria, suspended solids and residual oil. Each of these factors accelerates metal loss, and the damage is usually concentrated at the connection, near the packer and along the section where the tubing string rubs against the casing wall. Field experience shows that corrosion is rarely caused by one aggressive medium alone; it develops when poor water quality, mechanical damage and an unprotected annulus act together. For this reason, an anti-corrosion programme for OCTG casing must be built as a system of measures rather than as a single product choice.

The practical goal is to keep the annular space free of oxygen and bacteria, to avoid scratching the internal surface of the casing, and to leave room for upgrading the material or applying external protection once the basic water treatment is under control.

Step 1: Water Quality Control and Source Management

Water quality is the first and least expensive lever. Injection water should be treated so that dissolved oxygen, bacteria, iron, oil and suspended solids stay within the targets set for the reservoir, and the quality must be verified at the station and again at the wellhead. A typical waterflood quality window used in the industry is summarised below; the exact limits are agreed between the operator and the reservoir engineer for each field.

Parameter Typical target for injection water Effect if exceeded
Dissolved oxygen Below 0.02 mg/L at the wellhead Pitting corrosion of carbon steel casing
Sulphate-reducing bacteria Below 10 cells/mL Souring, localised pitting and H2S generation
Total iron Below 0.5 mg/L Deposits and under-deposit corrosion
Suspended solids Below 5 mg/L, filtered to reservoir pore size Plugging and differential aeration cells
Oil content Below 10 mg/L Bacterial growth and biofilm
pH 6.5 to 8.5 Acid attack at low pH, scaling at high pH

Measures that support these targets include closed water injection circuits, oxygen scavenger dosing, biocide treatment on a planned schedule, filtration, and separate cleaning and injection of the main water pipelines. Strengthening the cleaning of the trunk lines and of the station equipment reduces the volume of corrosion products that would otherwise be carried into the annular space of every well on the pattern.

Step 2: Annular Protection Fluid

For a newly commissioned injection well, annular protection fluid is the primary barrier between the outside surface of the tubing and the inside surface of the casing. The fluid is formulated with a corrosion inhibitor and is added on a fixed schedule rather than on an ad hoc basis. A written dosing system should define the volume per treatment, the interval, the target inhibitor concentration measured in the returns, and the person responsible for each step. Monitoring of inhibitor residual concentration and of iron content in the annular fluid provides evidence that the treatment is actually working.

Use a clean, filtered base fluid compatible with the packer elastomers.

Maintain a defined inhibitor residual in the annulus at all times.

Record volume, concentration and date for every treatment.

Sample the annulus at least quarterly and trend the iron content.

Step 3: Mechanical Protection of the Casing String

Mechanical scratches remove the protective scale layer and create fresh anodic sites that are far more corrosive than the undisturbed surface. In deviated wells the tubing string tends to lie against the casing wall, and the coupling is the contact point. Two simple countermeasures are widely used:

Fit a rubber ring at the tubing coupling to cushion the contact between tubing and casing.

Install centralisers in strongly deviated sections so that the string is kept away from the wall.

These items are low cost, but they must be sized for the actual casing inside diameter and the completion load, and they must be installed during the workover, because retrofitting is usually impractical. Torque and drag calculations should confirm that the added centralisers do not create an excessive running load.

Step 4: Cathodic Protection and Coated Casing

Cathodic protection and internal or external coated casing are effective technologies, but they are not the first step in a water injection well. Until water quality, annular fluid management and mechanical protection are under control, installing coated casing in a well that still receives oxygen-rich or bacteria-laden water only moves the corrosion to the uncoated areas, particularly at connections. The recommended sequence is therefore to stabilise the water treatment, continue monitoring, and then evaluate coating or cathodic protection if the corrosion rate remains above the accepted limit. Where the produced or injected fluid contains hydrogen sulphide or carbon dioxide, material selection should follow ISO 15156 (NACE MR0175) and casing grades such as the API 5CT L80 Type 1, L80 13Cr, C90, T95 or C110 families can be considered as part of a corrosion-resistant completion.

Step 5: Monitoring, Records and Review

An anti-corrosion programme without measurement cannot be managed. Recommended practice is to combine water analysis, inhibitor residual checks, iron counts, caliper or ultrasonic wall-thickness logging and annulus pressure monitoring into one trend sheet per well. A rising iron count or a change in annulus pressure is the earliest reliable warning of casing damage. Where the water injection well is completed with alloy or high-temperature pipe, the same discipline applies: the grade actually delivered, for example an ASTM A335 P5, P11, P22 or P91 pipe, must be verified against the mill certificate before installation so that the corrosion allowance is calculated on the real material rather than on the ordered one.

FAQ

Q: What is the single most important anti-corrosion measure for OCTG casing in a water injection well?
Keeping dissolved oxygen and sulphate-reducing bacteria out of the injected water and out of the annulus, because both drive pitting corrosion of carbon steel.

Q: Should cathodic protection be installed at the start of injection?
No. It is normally deferred until water quality, annular protection fluid and mechanical protection are stable and the measured corrosion rate is still too high.

Q: How do centralisers reduce casing corrosion?
They keep the tubing string away from the casing wall in deviated sections, so the protective scale layer is not scratched away and fresh anodic sites are not exposed.

Q: How often should annular protection fluid be added?
On a fixed schedule defined in the well programme, usually monthly or quarterly, with inhibitor residual and iron content measured at each treatment.

Q: Which casing grades are used when the fluid is sour?
Sour service material selection follows ISO 15156 (NACE MR0175); API 5CT corrosion-resistant grades such as L80 Type 1, L80 13Cr, C90, T95 and C110 are common choices.

Q: Can coated casing solve the problem on its own?
No. Coating protects the coated length but leaves connections and damaged areas exposed, so it is used together with water treatment and annular fluid control rather than instead of them.