St45.8 is a grade of the German standard DIN 17175, which is a carbon steel pipe.
Chemical properties of St45.8 seamless pipes
| component | C | Si ① | Mn | P | S |
|---|---|---|---|---|---|
| Min | - | 0.1 | 0.4 | - | - |
| Max | 0.21 | 0.35 | 1.2 | 0.04 | 0.04 |
Mechanical properties of St45.8 seamless pipes
| Wall Thickness t mm |
Tensile Strength σb Mpa |
Yield Point σs Mpa |
Elongation at break or elongation δ % |
Shock absorbed energy KV2 J |
|---|---|---|---|---|
| t≤16 | 410~530 | ≥255ⓐ | L0=5d0 Longitudinal: ≥21 Horizontal:≥19 |
DVM Sample Horizontal:≥27ⓑ |
| 16<t≤40 | 410~530 | ≥245ⓐ | L0=5d0 Longitudinal: ≥21 Horizontal:≥19 |
DVM Sample Horizontal:≥27ⓑ |
| 40<t≤60 | 410~530 | ≥235* | L0=5d0 Longitudinal: ≥21 Horizontal:≥19 |
DVM Sample Horizontal:≥27ⓑ |
ⓐ For tubes with an outside diameter ≤ 30 mm and a wall thickness ≤ 3 mm, the minimum value, to be 10 N/mm² lower.
ⓑ When examining longitudinal specimens (see Section 8-5-3), the minimum value for the notched impact toughness test, to be 14 Joules higher.
*The yield limit value for tubes made of this grade of steel, when the wall thickness is >60 mm, shall be determined by negotiation.
Minimum value of 0.2% yield point for ST45.8 seamless steel tubes at elevated temperatures
| Type | Wall Thickness (mm) |
0.2 per cent yield point at the following temperatures | ||||||||
| Grade | No | 200℃ | 250℃ | 300℃ | 350℃ | 400℃ | 450℃ | 500℃ | 550℃ | |
| MPa(Newtons/mm²) Min |
||||||||||
| St 45.8 | 1.0405 | ≤16 16<S≤40 40<S≤60¹ |
205 195 190 |
185 175 170 |
160 155 150 |
140 135 135 |
130 130 130 |
125 125 125 |
- | - |